1. Longitudinal cracks
The cracks are axial and thin and long in shape. When the mold is completely quenched, that is, centerless quenching, the core transforms into quenched martensite with the largest specific volume, generating tangential tensile stress. The higher the carbon content of the mold steel, the greater the tangential tensile stress generated. When the tensile stress When the strength limit of the steel is exceeded, longitudinal cracks will form. The following factors intensify the occurrence of longitudinal cracks: (1) The steel contains a large amount of low-melting point harmful impurities such as S, P, Sb, Bi, Pb, Sn, As, etc., and the steel ingot is severely segregated longitudinally along the rolling direction during rolling. , it is easy to cause stress concentration to form longitudinal quenching cracks, or the longitudinal cracks formed by rapid cooling of the raw material after rolling are not processed and retained in the product, causing the final quenching cracks to expand and form longitudinal cracks; (2) The mold size is within the quenching crack sensitive size range of steel. Longitudinal cracks are likely to form when the quenching cooling medium is selected (the dangerous size for quenching cracks is 8-15mm for carbon tool steel and 25-40mm for medium and low alloy steel) or when the selected quenching cooling medium greatly exceeds the critical quenching cooling rate of the steel.
Preventive measures: (1) Strictly inspect the raw materials when entering the warehouse, and do not put steel products with harmful impurity content into production; (2) Try to use vacuum smelting, out-of-furnace refining or electroslag remelting mold steel; (3) Improve the heat treatment process and use vacuum heating , protective atmosphere heating and sufficient deoxidation salt bath heating and graded quenching and isothermal quenching; (4) changing unintentional quenching to intentional quenching, that is, incomplete quenching, obtaining a strong and tough lower bainite structure and other measures, greatly reducing the tensile strength stress, which can effectively avoid longitudinal cracking and quenching distortion of the mold.
2. Transverse cracks
The crack characteristics are perpendicular to the axial direction. In unhardened molds, there is a large tensile stress peak in the transition between the hardened zone and the unhardened zone. When a large mold is rapidly cooled, a large tensile stress peak is easily formed. Because the axial stress formed is greater than the tangential stress, resulting in lateral stress. crack. S, P. in the forging module. Lateral segregation of harmful impurities with low melting points such as Sb, Bi, Pb, Sn, As, etc. or transverse microscopic cracks in the module, which expand to form transverse cracks after quenching.
Preventive measures: (1) The module should be reasonably forged. The ratio of raw material length to diameter, that is, the forging ratio, is preferably between 2 and 3. Double cross-shaped direction change forging is used for forging, and it is forged with five upsetting, five drawings and multiple fires to make the steel in the center. The carbides and impurities are fine and small, evenly distributed in the steel matrix, and the forging fiber structure is distributed non-directionally around the cavity, which greatly improves the transverse mechanical properties of the module and reduces and eliminates stress sources; (2) Choose the ideal cooling rate and cooling medium : Rapid cooling above the Ms point of the steel, greater than the critical quenching cooling rate of the steel, the stress generated by the supercooled austenite in the steel is thermal stress, the surface layer is compressive stress, and the inner layer is tensile stress, canceling each other out, effectively preventing thermal stress Cracks are formed and slowly cooled between Ms-Mf of the steel, which greatly reduces the organizational stress when forming quenched martensite. When the sum of thermal stress and corresponding stress in the steel is positive (tensile stress), it is easy to quench and crack. When it is negative, it is not easy to quench and crack. Making full use of thermal stress, reducing phase change stress, and controlling the sum of stresses to be negative can effectively avoid the occurrence of transverse quenching cracks. CL-1 organic quenching medium is an ideal quenching agent, which can reduce and avoid the distortion of the quenching mold and control the reasonable distribution of the hardened layer. By adjusting the different concentration ratios of CL-1 quenching agent, different cooling rates can be obtained, and the required hardened layer distribution can be obtained to meet the needs of different mold steels.
3. Arc cracks
It often occurs at sudden shape changes such as mold corners, notches, holes, and die wiring flash. This is because the stress generated at the edges and corners during quenching is 10 times the average stress on the smooth surface. In addition, (1) the higher the carbon (C) content and alloying element content in the steel, the lower the Ms point of the steel. If the Ms point decreases by 2°C, the quenching cracking tendency will increase by 1.2 times. If the Ms point decreases by 8°C, the quenching cracking tendency will increase. The tendency increases by 8 times; (2) The transformation of different structures in steel and the transformation of the same structure are not simultaneous. Due to the specific tolerance of different structures, huge structural stress is caused, resulting in the formation of arc-shaped cracks at the junction of the structures; (3) Failure to respond in time after quenching Fire, or insufficient tempering, the retained austenite in the steel is not fully transformed and remains in the service state, promoting stress redistribution, or the retained austenite undergoes martensitic transformation to generate new internal stress when the mold is in service. When the comprehensive stress is greater than the strength limit of the steel, arc-shaped cracks will form; (4) It has the second type of temper brittle steel. After quenching, it is tempered at high temperature and cooled slowly, causing harmful impurity compounds such as P and s in the steel to precipitate along the grain boundaries, greatly reducing the The grain boundary bonding force and strong toughness increase the brittleness and form arc-shaped cracks under the action of external forces during service.
Preventive measures: (1) Improve the design, try to make the shape as symmetrical as possible, reduce shape mutations, add process holes and reinforcement ribs, or use combined assembly; (2) Replace right angles and sharp edges with rounded corners, replace blind holes with through holes, and improve Processing accuracy and surface finish reduce stress concentration sources. Generally, hardness requirements are not high for unavoidable right angles, sharp edges, blind holes, etc. Iron wire, asbestos rope, refractory mud, etc. can be used for wrapping or filling to create artificial cooling barriers. Allow it to be cooled and quenched slowly to avoid stress concentration and prevent the formation of arc-shaped cracks during quenching; (3) The quenched steel should be tempered in time to eliminate part of the quenching internal stress and prevent the quenching stress from expanding; (4) Tempering for a longer period of time can improve the mold resistance. Fracture toughness value; (5) Full tempering to obtain stable microstructure and properties; (6) Multiple tempering to fully transform the retained austenite and eliminate new stress; (7) Reasonable tempering to improve the fatigue resistance of steel parts and comprehensive mechanical properties. Mechanical properties; (8) For mold steel with type II temper brittleness, it should be cooled quickly (water cooling or oil cooling) after high temperature tempering, which can eliminate the type II temper brittleness and prevent and avoid the formation of arc cracks during quenching.
4. Peeling cracks
When the mold is in service, under the action of stress, the quenched hardened layer peels off from the steel matrix piece by piece. Because the specific volumes of the surface tissue and the core tissue of the mold are different, axial and tangential quenching stresses are formed on the surface during quenching, and tensile stress is generated in the radial direction, which suddenly changes to the inside. Peeling cracks occur in narrow areas where the range of rapid stress changes is narrow, which often occurs in During the cooling process of the surface chemical heat treatment mold, the quenching martensitic expansion of the inner and outer layers does not proceed at the same time due to the synchronicity between the chemical modification of the surface layer and the phase transformation of the steel matrix, resulting in a large phase transformation stress, causing the chemically treated infiltration layer to separate from the matrix structure. Strip. Such as flame surface hardening layer, high frequency surface hardening layer, carburizing layer, carbonitriding layer, nitriding layer, boronizing layer, metallizing layer, etc. It is not advisable to temper quickly after quenching the chemical permeable layer, especially if the low temperature tempering is heated below 300~C and is heated quickly, it will cause the formation of tensile stress in the surface layer, while the core of the steel matrix and the transition layer will form compressive stress. When the tensile stress is greater than the compressive stress, it will cause The chemically penetrated layer was pulled apart and peeled off.
Preventive measures: (1) The concentration and hardness of the chemically infiltrated layer of mold steel should be gradually reduced from the surface to the inside to enhance the bonding force between the chemically infiltrated layer and the matrix. Diffusion treatment after infiltration can make the transition between the chemically infiltrated layer and the matrix uniform; (2) Mold Before chemical treatment of steel, diffusion annealing, spheroidizing annealing, and quenching and tempering are performed to fully refine the original structure, which can effectively prevent and avoid the occurrence of peeling cracks and ensure product quality.
5. Network cracks
The depth of the cracks is shallow, generally about 0.01-1.5mm deep, radiating, also known as cracks. The main reasons are: (1) The raw material has a deep decarburization layer that is not removed by cold cutting, or the finished mold is heated in an oxidizing atmosphere furnace to cause oxidative decarburization; (2) The metal structure of the decarburized surface layer of the mold is different from the martensite of the steel matrix. Different carbon contents and different specific volumes produce large tensile stress when the decarburized surface layer of steel is quenched. Therefore, the surface metal is often pulled into a network along the grain boundaries; (3) The raw material is coarse-grained steel, and the original structure is coarse. There are large pieces of ferrite that cannot be eliminated by conventional quenching and remain in the quenched structure, or the temperature control is inaccurate, the instrument fails, the structure overheats, or even overburns, the grains become coarsened, the grain boundary bonding force is lost, and the mold is quenched and cooled When the steel carbides precipitate along the austenite grain boundaries, the strength of the grain boundaries is greatly reduced, the toughness is poor, and the brittleness is high. Under the action of tensile stress, the steel will crack in a network shape along the grain boundaries.
Preventive measures: (1) Strict the chemical composition of raw materials. Metallographic structure and flaw detection inspection, unqualified raw materials and coarse-grained steel are not suitable as mold materials; (2) Use fine-grained steel and vacuum electric furnace steel, recheck the depth of the decarburized layer of the raw material before putting into production, and the cold cutting machining allowance must be greater than the decarburized layer. Carbon layer depth; (3) Develop an advanced and reasonable heat treatment process, use microcomputer temperature control instruments, the control accuracy reaches 1.5°C, and regularly calibrate the instruments on site; (4) Use vacuum electric furnaces, protective atmosphere furnaces and fully deoxidized salts for final treatment of mold products Bath furnace heating mold products and other measures can effectively prevent and avoid the formation of network cracks.
picture
6. Cold treatment cracks
Most of the mold steels are medium and high carbon alloy steels. After quenching, there is still some supercooled austenite that has not been transformed into martensite and remains in the use state as retained austenite, which affects the performance. If it is placed below zero and continued to cool, it can promote the martensitic transformation of the retained austenite. Therefore, the essence of cold treatment is to continue quenching. The quenching stress at room temperature and the quenching stress at zero are superimposed. When the superposition stress exceeds the strength limit of the material, cold treatment cracks will form.
Preventive measures: (1) Place the mold in boiling water for 30-60 minutes before cold treatment after quenching, which can eliminate 15%-25% of the quenching internal stress and stabilize the retained austenite, and then perform conventional cold treatment at -60°C, or perform -120℃ cryogenic treatment, the lower the temperature, the more retained austenite will be transformed into martensite, but it is impossible to complete the transformation. Experiments show that about 2%-5% of the retained austenite remains, and it can be retained as needed. A small amount of retained austenite can relax stress and play a buffering role. Because the retained austenite is soft and tough, it can partially absorb the sharp expansion energy of martensite and ease the phase transformation stress; (2) After the cold treatment, take out the mold and put it into the heat Heating in water can eliminate 40%-60% of the cold treatment stress. After heating to room temperature, it should be tempered in time to further eliminate the cold treatment stress, avoid the formation of cold treatment cracks, obtain stable organizational properties, and ensure that the mold product does not suffer distortion during storage and use.
7. Grinding cracks
It often occurs during the cold grinding process of the finished mold after quenching and tempering. Most of the micro cracks formed are perpendicular to the grinding direction and are about 0.05-1.0mm deep. (1) Improper pretreatment of raw materials, failure to fully eliminate block, network, and band carbides in raw materials and severe decarburization; (2) The final quenching heating temperature is too high, overheating occurs, the grains are coarse, and more residues are generated Austenite; (3) Stress-induced phase transformation occurs during grinding, causing the residual austenite to transform into martensite. The structural stress is large, and due to insufficient tempering, more residual tensile stress remains, which is incompatible with the grinding process. The superposition of stress in the cutting structure, or due to high grinding speed, large feed amount, and improper cooling, cause the grinding heat of the metal surface to rise sharply to the quenching heating temperature, and then the grinding fluid cools, resulting in secondary quenching of the grinding surface and various stresses. In summary, if the strength limit of the material is exceeded, grinding cracks in the surface metal will be caused.
Preventive measures: (1) Modify the raw material and perform multiple double cross-shaped upsetting and forging processes. After four upsetting and four drawings, the forged fiber structure is symmetrically distributed in a wave shape around the cavity or axis, and the high-temperature waste heat of the last fire is used. Quenching, followed by high-temperature tempering, can fully eliminate massive, reticular, ribbon and chain carbides and refine the carbides to 2-3 levels; (2) Develop an advanced heat treatment process to control the final quenching residual alkali The stenite content does not exceed the standard; (3) Temper in time after quenching to eliminate quenching stress; (4) Appropriately reduce the grinding speed, grinding amount, and grinding cooling rate, which can effectively prevent and avoid the formation of grinding cracks.
8. Wire cutting cracks
This crack occurs during the online cutting process of the quenched and tempered module. This process changes the stress field distribution state of the metal surface layer, middle layer and core. The quenching residual internal stress loses balance and deforms, and a large tensile stress appears in a certain area. , this tensile stress reaches the strength limit of the mold material, causing it to explode. The crack is an arc tail-shaped rigid metamorphic layer crack. Experiments show that the wire cutting process is a process of local high-temperature discharge and rapid cooling, which causes the metal surface to form a solidified layer of dendritic cast structure, producing a tensile stress of 600-900MPa and a high-stress secondary quenching white layer about 0.03mm thick. Reasons for cracks: (1) There is severe carbide segregation in the raw materials; (2) Instrument failure, the quenching heating temperature is too high, and the grains are coarse, which reduces the strength and toughness of the material and increases the brittleness; (3) The quenched workpiece is not tempered and tempered in time. Insufficient fire, excessive residual internal stress and the superposition of new internal stress formed during the wire cutting process lead to wire cutting cracks.
Preventive measures: (1) Strict inspection of raw materials before storage to ensure that the structural composition of the raw materials is qualified. Unqualified raw materials must be forged to break the carbides so that the chemical composition, metallographic structure, etc. meet the technical conditions before being put into production. Before the module heat treatment, the finished product must be left with a certain amount of grinding and then quenched. Tempering and wire cutting; (2) Check the instrument before entering the furnace, use microcomputer temperature control, the temperature control accuracy is 1.5°C, vacuum furnace, protective atmosphere furnace heating, strictly prevent overheating and oxidative decarburization; (3) Use graded quenching, isothermal Quenching and tempering in time after quenching and multiple temperings can fully eliminate internal stress and create conditions for wire cutting; (4) Develop a scientific and reasonable wire cutting process.
9. Fatigue fracture
Microscopic fatigue cracks formed under the repeated action of alternating stress during mold service slowly expand, leading to sudden fatigue fracture. (1) The raw materials have hair lines, self-points, pores, looseness, non-metallic inclusions, severe segregation of carbides, banded structures, and massive free ferrite metallurgical structural defects, which destroy the continuity of the matrix structure and form uneven stress concentrations. . 112 is not removed from the steel ingot, resulting in the formation of white spots during rolling. There are harmful impurities such as Sb, Bi, Pb, Sn, As, S, and P in steel. P in steel can easily cause cold brittleness, while s can easily cause hot brittleness. Excessive S and P harmful impurities can easily form fatigue sources; (2 ) The chemical penetration layer is too thick, the concentration is too high, the penetration layer is too shallow, the hardening layer is too shallow, and the hardness of the transition zone is low, etc., which can lead to a sharp reduction in the fatigue strength of the material; (3) When the mold surface is rough, the precision is low, the finish is poor, and Knife marks, lettering, scratches, bumps, corrosion pitting, etc. can also easily cause stress concentration and lead to fatigue fracture.
Preventive measures: (1) Strictly select materials to ensure quality, and control the content of low melting point impurities such as Pb, As, Sn, and S, P non-metallic impurities to not exceed the standard; (2) Conduct material inspection before production, and unqualified raw materials will not be put into production; (3) ) Choose materials with high purity, few impurities, uniform chemical composition and fine grains. Electroslag remelted refined steel with the characteristics of small carbides, good isotropic properties and high fatigue strength is shot peened and strengthened on the surface of the mold surface and the surface chemical permeation layer is modified and strengthened to make the metal surface pre-stressed and offset the mold. The tensile stress generated during service improves the fatigue strength of the mold surface; (4) improves the processing accuracy and smoothness of the mold surface; (5) improves the structural properties of the chemical permeable layer and hardened layer; (6) uses a microcomputer to control the thickness of the chemical permeable layer, concentration and hardened layer thickness.
10. Stress corrosion cracking
This crack often occurs during use. The metal mold cracks due to chemical reaction or electrochemical reaction process, which causes damage and corrosion from the surface to the internal structure. This is stress corrosion cracking. Due to the different structures of mold steel after heat treatment, the corrosion resistance properties are also different. The most corrosion-resistant structure is austenite (A), the most corrosion-resistant structure is troostite (T), and the order is ferrite (F) - martensite (M) - pearlite (P) - sorbite ( S). Therefore, it is not suitable to obtain T group by heat treatment of mold steel.
Weave. Although the quenched steel has been tempered, due to insufficient tempering, the quenching internal stress still exists more or less. New stress will also be generated under the action of external forces when the mold is in service. Whenever there is stress in the metal mold, there will be stress. Corrosion cracks occur.
Preventive measures: (1) After quenching, mold steel should be tempered in time, fully tempered, and tempered multiple times to eliminate the internal stress of quenching; (2) After quenching, mold steel should generally not be tempered at 350-400~C due to the T structure. It often occurs at this temperature, and the mold with T structure should be reprocessed. The mold should be rust-proofed to improve the corrosion resistance; (3) Low-temperature preheating should be performed before the hot-work mold is put into service, and a low-temperature preheating should be performed after the cold-work mold has been in service for a period. Tempering to eliminate stress can not only prevent and avoid the occurrence of stress corrosion cracks, but also greatly increase the service life of the mold. It kills two birds with one stone and has significant technical and economic benefits.