⑴ The shape and wall thickness of the plastic part should be designed to facilitate the smooth flow of material to fill the cavity, and try to avoid sharp corners and gaps.
⑵ The draft angle should be large, 1° to 2° for a mold containing 15% glass fiber, and 2° to 3° for a mold containing 30% glass fiber. When the demoulding slope is not allowed, forced demoulding should be avoided and a transverse parting structure should be used.
⑶The cross-section of the pouring system should be large, and the process should be straight and short to facilitate the even dispersion of fibers.
⑷ When designing the feed inlet, consideration should be given to preventing insufficient filling, anisotropic deformation, uneven distribution of glass fibers, and easy generation of weld marks and other adverse consequences. The feed port should be thin, wide, fan-shaped, annular or multi-point in order to make the material flow turbulent and the glass fiber evenly dispersed to reduce anisotropy. It is best not to use a needle-shaped feed port. The mouth section can be appropriately increased, and its length should be short.
⑸The mold core and cavity should have sufficient rigidity and strength.
⑹ The mold should be hardened, polished and made of wear-resistant steel, and the easily worn parts should be easy to repair.
⑺The ejection should be uniform and powerful to facilitate replacement and repair.
⑻The mold should be equipped with an exhaust overflow tank and should be located in a location prone to weld marks.
Mold temperature setting
⑴Mold temperature affects the molding cycle and molding quality. In actual operation, the mold temperature is set starting from the lowest appropriate mold temperature of the material used, and then is adjusted appropriately according to the quality condition.
⑵Correctly speaking, mold temperature refers to the temperature of the mold cavity surface when molding is in progress. In mold design and molding engineering conditions setting, it is important not only to maintain an appropriate temperature, but also to distribute it evenly. .
⑶ Uneven mold temperature distribution will lead to uneven shrinkage and internal stress, thus making the molding port prone to deformation and warping. picture
⑷Increasing the mold temperature can achieve the following effects;
① Increase the crystallinity and more uniform structure of molded products.
② Make the molding shrinkage more sufficient and reduce the post-shrinkage.
③Improve the strength and heat resistance of molded products.
④ Reduce internal stress residual, molecular alignment and deformation.
⑤ Reduce flow resistance during filling and reduce pressure loss.
⑥Make the appearance of the molded product more shiny.
⑦ Increase the chance of burrs occurring in molded products.
⑧Increase the chance of dents near the gate and reduce the chance of dents far from the gate.
⑨ Reduce the obvious degree of joint lines
⑩Increase the cooling time.
Dosing and plasticization
⑴In the molding process, the plasticizing unit of the injection machine is responsible for the control (metering) of the injection volume and the uniform melting (plasticization) of the plastic.
①Heating barrel temperature (Barrel Temperature)
Although about 60-85% of the melting of plastic is due to the heat energy generated by the rotation of the screw, the melting state of the plastic is still affected by the temperature of the heating barrel, especially the temperature near the front area of the nozzle - the temperature in the front area is too high When it is high, it is easy to cause material dripping and string pulling when taking out the parts.
②Screw speed
A. The melting of plastic is generally due to the heat generated by the rotation of the screw. Therefore, if the screw rotates too fast, it will have the following effects:
a. Thermal decomposition of plastics.
b. Glass fiber (fiber-added plastic) is shortened.
c. The screw or heating barrel wears faster.
B. The setting of rotation speed can be measured by the size of its circumferential speed:
Circumferential speed = n (rotation speed) * d (diameter) * π (circumferential ratio)
Generally, for plastics with low viscosity and good thermal stability, the peripheral speed of the screw rod rotation can be set to about 1m/s, but for plastics with poor thermal stability, it should be as low as about 0.1.
C. In practical applications, we can lower the screw speed as much as possible so that the rotating feed can be completed before mold opening.
③Back pressure (BACK PRESSURE)
A. When the screw rotates and feeds material, the pressure accumulated by the melt pushed to the front end of the screw is called back pressure. During injection molding, it can be adjusted by adjusting the oil withdrawal pressure of the injection hydraulic cylinder. The back pressure can be as follows Effect:
a. The melt melts more uniformly.
b. Colorants and fillers are dispersed more evenly.
c. Let the gas exit from the blanking port.
d. Accurate measurement of feed materials.
B. The level of back pressure is determined by the viscosity and thermal stability of the plastic. Too high back pressure will prolong the feeding time and easily cause the plastic to overheat due to the increase in rotational shear force. Generally, 5--15kg/cm2 is appropriate.
④SUCK BACK, DECOMPRESSION
A. Before the screw rotates and feeds, the screw is properly withdrawn to reduce the melt pressure at the front end of the mold. This is called front loosening. Its effect can prevent the melt at the nozzle from exerting pressure on the screw. It is mostly used in hot runners. Mold forming.
B. After the screw rotation and feeding are completed, the screw is properly withdrawn to reduce the melt pressure at the front end of the screw. This is called back-retraction, and its effect can prevent dripping at the nozzle.
C. The disadvantage is that it is easy for the main channel (SPRUE) to stick to the mold; too much looseness can suck in air and cause air marks in the molded product.